耐蚀合金: 耐蚀合金是一种特殊的不锈钢,首先在化学成分上与普通不锈钢不同,是指含高镍,高铬,高钼的一种高合金不锈钢。其次在耐高温或者耐腐蚀的性能上,与普通不锈钢相比,具有更加优秀的耐高温或者耐腐蚀性能,在许多的领域中,比如:
1,海洋:海域环境的海洋构造物,海水淡化,海水养殖,海水热交换等。
2,环保领域:火力发电的烟气脱硫装置,废水处理等。
3,能源领域:原子能发电,煤炭的综合利用,海潮发电等。
4,石油化工领域:炼油,化学化工设备等。
5,食品领域:制盐,酱油酿造等。
铁基耐蚀合金化学成分:
牌号 |
C |
Cr |
Ni |
Mo |
Co |
Cu |
Al |
Ti |
Fe |
Si |
Mn |
P |
S |
其他 |
NS111 Incoloy800 |
≤0.10 |
19.0~23.0 |
30.0~35.0 |
- |
- |
≤0.75 |
0.15~0.60 |
0.15~0.60 |
余 |
≤1.00 |
≤1.50 |
≤0.030 |
≤0.015 |
- |
NS112 Incoloy800H |
0.05~0.10 |
19.0~23.0 |
30.0~35.0 |
- |
- |
≤0.75 |
0.15~0.60 |
0.15~0.60 |
余 |
≤1.00 |
≤1.50 |
≤0.030 |
≤0.015 |
- |
NS113 |
≤0.030 |
24.0~26.5 |
34.0~37.0 |
- |
- |
- |
0.15~0.45 |
0.15~0.60 |
余 |
0.30~0.70 |
0.50~1.50 |
≤0.030 |
≤0.030 |
- |
NS131 |
≤0.05 |
19.0~21.0 |
42.0~44.0 |
12.5~13.5 |
- |
- |
- |
- |
余 |
≤0.70 |
≤1.00 |
≤0.030 |
≤0.030 |
- |
NS141 |
≤0.030 |
25.0~27.0 |
34.0~37.0 |
2.0~3.0 |
- |
3.0~4.0 |
- |
0.40~0.90 |
余 |
≤0.70 |
≤1.00 |
≤0.030 |
≤0.030 |
- |
NS142 Incoloy825 |
≤0.05 |
19.5~23.5 |
38.0~46.0 |
2.5~3.5 |
- |
1.5~3.0 |
≤0.20 |
0.60~1.20 |
余 |
≤0.50 |
≤1.00 |
≤0.030 |
≤0.030 |
- |
NS143 Alloy20Cb |
≤0.07 |
19.0~21.0 |
32.0~38.0 |
2.0~3.0 |
- |
3.0~4.0 |
- |
- |
余 |
≤1.00 |
≤2.00 |
≤0.030 |
≤0.030 |
Nb8×C~1.00 |
铁基耐蚀合金力学性能:
牌号 |
固溶处理 温度/℃ |
抗拉强度 σb / MPa |
屈服强度 σ0.2 / MPa |
伸长率 δ5(%) |
不 小 于 |
NS111 |
1000~1060 |
515 |
205 |
30 |
NS112 |
1100~1170 |
450 |
170 |
30 |
NS113 |
1000~1050 |
515 |
205 |
30 |
NS131 |
1150~1200 |
590 |
240 |
30 |
NS141 |
1000~1050 |
540 |
215 |
35 |
NS142 |
1000~1050 |
590 |
240 |
30 |
NS143 |
1000~1050 |
540 |
215 |
35 |
铁基耐蚀合金性能特点及用途:
牌号 |
性能特点 |
用途举例 |
NS111 |
抗氧化性介质腐蚀,高温下抗渗碳性良好 |
热交换器及蒸汽发生器管、合成纤维的加热管 |
NS112 |
抗氧化性介质腐蚀,抗高温渗碳,热强度高 |
合成纤维工程中的加热管、炉管及耐热构件等 |
NS113 |
耐高温高压水的应力腐蚀及苛性介质应力腐蚀 |
核电站的蒸汽发生器管 |
NS131 |
在含卤素离子氧化-还原复合介质中耐点腐蚀 |
湿法冶金、制盐、造纸及合成纤维工业的含氯离子环境 |
NS141 |
耐氧化-还原介质腐蚀及氯化物介质的应力腐蚀 |
硫酸及含有多种金属离子和卤族离子的硫酸装置 |
NS142 |
耐氧化物应力腐蚀及氧化-还原性复合介质腐蚀 |
热交换器及冷凝器、含多种离子的硫酸环境 |
NS143 |
耐氧化-还原性复合介质腐蚀 |
硫酸环境及含有卤族离子及金属离子的硫酸溶液中应用,如湿法冶金及硫酸工业装置 |
镍基耐蚀合金化学成分:
牌号 |
C |
Cr |
Ni |
Mo |
Co |
Cu |
Al |
Ti |
Fe |
Si |
Mn |
P |
S |
其他 |
NS311 |
≤0.06 |
28.0~ 31.0 |
余 |
- |
- |
- |
≤0.30 |
- |
≤1.0 |
≤0.50 |
≤1.20 |
≤0.020 |
≤0.020 |
- |
NS312 |
≤0.15 |
14.0~ 17.0 |
余 |
- |
- |
≤0.50 |
- |
- |
6.0~ 10.0 |
≤0.50 |
≤1.00 |
≤0.030 |
≤0.015 |
- |
NS313 |
≤0.10 |
21.0~ 25.0 |
余 |
- |
- |
≤1.00 |
1.00/1.70 |
- |
10.0~15.0 |
≤0.05 |
≤1.00 |
≤0.030 |
≤0.015 |
- |
NS314 |
≤0.030 |
35.0~ 38.0 |
余 |
- |
- |
- |
0.20/0.50 |
- |
≤1.0 |
≤0.50 |
≤1.00 |
≤0.030 |
≤0.020 |
- |
NS315 |
≤0.05 |
27.0~ 31.0 |
余 |
- |
- |
≤0.50 |
- |
- |
7.0~ 11.0 |
≤0.50 |
≤0.50 |
≤0.030 |
≤0.015 |
- |
NS321 哈B |
≤0.05 |
≤1.00 |
余 |
26.0~30.0 |
≤2.5 |
- |
- |
- |
4.0~ 6.0 |
≤1.00 |
≤1.00 |
≤0.030 |
≤0.030 |
V0.20~0.40 |
NS322 哈B-2 |
≤0.020 |
≤1.00 |
余 |
26.0~30.0 |
≤1.0 |
- |
- |
- |
≤2.0 |
≤1.00 |
≤1.00 |
≤0.040 |
≤0.030 |
- |
NS331 |
≤0030 |
14.0~ 17.0 |
余 |
2.0~ 3.0 |
- |
- |
- |
0.40~0.90 |
≤8.0 |
≤0.70 |
≤1.00 |
≤0.030 |
≤0.020 |
- |
NS332 |
≤0.030 |
17.0~ 19.0 |
余 |
16.0~18.0 |
- |
- |
- |
- |
≤1.0 |
≤0.70 |
≤1.00 |
≤0.030 |
≤0.030 |
- |
NS333 哈C |
≤0.08 |
14.5~ 16.5 |
余 |
15.0~17.0 |
≤2.5 |
- |
- |
- |
4.0~ 7.0 |
≤1.00 |
≤1.00 |
≤0.04 |
≤0.030 |
W3.0~4.5; V≤0.35 |
牌号 |
C |
Cr |
Ni |
Mo |
Co |
Cu |
N |
Ti |
Fe |
Si |
Mn |
P |
S |
其他 |
NS334哈C276 |
≤0.020 |
14.5~ 16.5 |
余 |
15.0~17.0 |
≤2.5 |
- |
- |
- |
4.0~ 7.0 |
≤0.08 |
≤1.00 |
≤0.040 |
≤0.030 |
W3.0~4.5; V≤0.35 |
NS335 |
≤0.015 |
14.0~ 18.0 |
余 |
14.0~17.00 |
≤2.0 |
- |
- |
≤0.70 |
≤3.0 |
≤0.08 |
≤1.00 |
≤0.040 |
≤0.030 |
- |
NS336 Inconel625 |
≤0.10 |
20.0~ 23.0 |
余 |
8.0~ 10.0 |
≤1.0 |
- |
≤0.40 |
≤0.40 |
≤5.0 |
≤0.50 |
≤0.50 |
≤0.015 |
≤0.015 |
Nb3.15~4.15 |
NS337 |
≤0.030 |
19.0~ 21.0 |
余 |
15.0~17.0 |
≤0.10 |
≤0.10 |
- |
- |
≤5.0 |
≤0.40 |
0.50/1.50 |
≤0.020 |
≤0.020 |
- |
NS341 |
≤0.030 |
19.0~ 21.0 |
余 |
2.0~3.0 |
- |
1.0~2.0 |
- |
0.4~0.9 |
≤7.0 |
≤0.70 |
≤1.00 |
≤0.030 |
≤0.030 |
- |
NS411 |
≤0.05 |
19.0~ 21.0 |
余 |
- |
- |
- |
0.40~1.00 |
2.25~2.75 |
5.0~9.0 |
≤0.80 |
≤1.00 |
≤0.030 |
≤0.030 |
Nb0.70~1.20 |
Monel400 |
0.12 |
|
65.00 |
|
|
32.00 |
|
|
1.50 |
|
1.00 |
|
|
|
MonelK500 |
0.13 |
|
64.00 |
|
|
30.00 |
|
0.60 |
|
|
0.80 |
|
|
Al 2.80 |
镍基耐蚀合金力学性能:
牌 号 |
固溶处理 温度/℃ |
抗拉强度 σb /MPa |
屈服强度 σ0.2 / MPa |
伸长率 δ5(%) |
冲击吸收功AKU/J |
硬度HRC |
不 小 于 |
- |
- |
NS311 |
1050~1100 |
570 |
245 |
40 |
- |
- |
NS312 |
1000~1050 |
550 |
240 |
30 |
- |
- |
NS313 |
1100~1150 |
550 |
195 |
30 |
- |
- |
NS314 |
1080~1120 |
520 |
195 |
35 |
- |
- |
NS315 |
1000~1050 |
550 |
240 |
30 |
- |
- |
NS321 |
1140~1190 |
690 |
310 |
40 |
- |
- |
NS322 |
1040~1090 |
760 |
350 |
40 |
- |
- |
NS331 |
1050~1100 |
540 |
195 |
35 |
- |
- |
NS332 |
1160~1210 |
735 |
295 |
30 |
- |
- |
NS333 |
1160~1210 |
690 |
315 |
30 |
- |
- |
NS334 |
1150~1200 |
690 |
285 |
40 |
- |
- |
NS335 |
1050~1100 |
690 |
275 |
40 |
- |
- |
NS336 |
1100~1150 |
690 |
275 |
30 |
- |
- |
NS341 |
1050~1100 |
590 |
195 |
40 |
- |
- |
NS411 |
1080~1100水冷 750~780×8h,空冷 620~650×8h,空冷 |
910 |
690 |
20 |
80 |
32 |
镍基耐蚀合金性能特点及用途:
类型 |
牌号 |
性能特点 |
用途举例 |
镍基耐蚀合金 |
NS311 |
抗强氧化性介质及含氟离子高温硝酸腐蚀,无磁 |
高温硝酸环境及强腐蚀条件下的无磁构件 |
NS312 |
耐高温氧化物介质腐蚀 |
热处理及化学加工工业装置 |
NS313 |
抗强氧化性介质腐蚀,高温强度高 |
强腐蚀性核工程废物烧结处理炉 |
NS314 |
耐强氧化性介质及高温硝酸、氢氟酸混合介质腐蚀 |
核工业中靶件及元件的溶解器 |
NS315 |
抗氯化物及高温高压水应力腐蚀,耐强氧化性介质及HNO,-HF混合腐蚀 |
核电站热交换器、蒸发器管、核工程化工后处理耐蚀构件 |
NS321 |
耐强还原性介质腐蚀 |
热浓盐酸及氯化氢气体装置及部件 |
NS322 |
耐强还原性介质腐蚀,改善抗晶间腐蚀性 |
盐酸及中等浓度硫酸环境(特别是高温下)的装置 |
NS331 |
耐高湿氟化氢、氯化氢气体及氟气腐蚀,易成形焊接 |
化工、核能及有色冶金中高温氟化氢炉管及容器 |
NS332 |
耐含氯离子的氧化-还原介质腐蚀,耐点腐蚀 |
湿氯、亚硫酸、次氯酸、硫酸、盐酸及氯化物溶液装置 |
NS333 |
耐卤族及其化合物腐蚀 |
强腐蚀性氧化-还原复合介质及高温海水中应用装置 |
NS334 |
耐氧化性氯化物水溶液及湿氯、次氯酸盐腐蚀 |
强腐蚀性氧化-还原复合介质及高温海水中的焊接构件 |
NS335 |
耐含氯离子的氧化-还原复合腐蚀,组织热稳定性好 |
湿氯、次氯酸、硫酸、盐酸、混合酸、氯化物装置,焊接后直接应用 |
NS336 |
耐氧化-还原复合介质、耐海水腐蚀,且热强度高 |
化学加工工业中苛刻腐蚀环境或海洋环境 |
NS337 |
焊接材料,焊接覆盖面大,耐苛刻环境腐蚀 |
多种高铬钼镍基合金的焊接及与不锈钢的焊接 |
NS341 |
耐含氟、氯离子的酸性介质的冲刷冷凝腐蚀 |
化工及湿法冶金冷凝器和炉管、容器 |
NS411 |
抗强氧化性介质腐蚀,可沉淀硬化,耐腐蚀冲击 |
硝酸等氧化性酸中工作的球阀及承载构件 |